Preparation:

1.Mesh: 30-60(12T-24T) to make thick screen by emulsion.

2.Pigments added ratio:2-4%

3.Catalyst mixing ratio:2%

4.Thinner XG-128AH adding ratio:0-10% thinner is not necessary

5.Heating Temp and time: 120℃ -150℃ for 6-12 seconds , Heating time depends on heating temp and printing size and thickness.

Silicone ink mixing tips:

Printing silicone   XG-15A 60G  

Catalyst    XG-15B  1.2G (2%)

Pigment   XG-1.2-2.4G (2-4%) If need color effect

To print by thick screen and big holes mesh for one layer then finish and heating by 120℃ -150℃ for 6-12 seconds , Heating time depends on heating temp and printing size and thickness.