How to print silicone for under wear bonding?
1.40-60(16T-24T) 65-75 degree Squeegee.
2.Catalyst mixing ratio:2-3%
3.Silicone thinner XG-128A adding ratio:20-40%
Heating Temp and Time: 110℃ for 15 minutes.
1.Screen printing silicone ink for underwear bonding printing:
2.Screen printing underwear bonding silicone print 1 layer:
Underwear bonding silicone XG-866NY 100G
Silicone thinner XG-128AH 20-40G 20-40%
Fast dry catalyst XG-866B-2 2-3G 2-3%
3.To stick a piece of underwear fabric on printed fabric, and smooth by tools3.Baking by 110℃ for 15 minutes.