Preparation

1.Mesh&Squeegee: 120(48T) Mesh number ;65-75 degree Squeegee.

2.Pigments added ratio:For white and fluorescent color 20%,other color 10%

3.Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.

4.Thinner XG-128A adding ratio:0-20% thinner is not necessary for hand printing

5.Heating Temp and time: Flash cure temp :100℃- 120℃ for 6-10 seconds ,Drying temp :120℃- 140℃ for about 2-5 minutes ,XG-360Z-1 and XG- 180AB have to to bake 10-20 minutes

Tips

1.Special agent for under coating for two times

A.Crossing lpasteer XG-360Z-3 20G (this is the new one)

Crossing lpasteer agent XG-360ZB 1G 5%

B.Adhesion agent XG-180A 20G

Adhesion agent harder XG-180B 2G 10 %

2.Two solutions can chose A or B depends on fabric type,need to do test first.

Cure by temp of 120℃ 10-20 seconds. Need longer curing time than silicone paste.

XG-180AB with better fastness and low cost than XG-360Z-1&XG-360ZB

1.HD silicone for under coating for 2-4 times

HD silicone XG-866A/866AH 30G(Or round silicone XG-866LK-1)

Thinner XG-128AH thinner is not necessary for hand printing,5-20% is enough for machine printing. Cure by temp of 120℃ 6-10 seconds.