Anti slip socks silicone paste New socks silicone paste testing

Preparation

1.Mesh: 30-60(12T-24T) to make thick screen by emulsion.Better to use Hollow aluminum plate as showed on video.

2.Pigments added ratio:2-4%

3.Catalyst mixing ratio:2%

4.Thinner XG-128AH adding ratio:thinner is not necessary

5.Heating Temp and time: 120℃ -150℃ for 6-12 seconds , Heating time depends on drying temp.

Silicone paste mixing tips

Socks silicone XG-15A+ 60G

Catalyst XG-15B+1.2G (2%)

Pigment XG- 1.2-2.4G (2-4%) If need color effect

To print by thick screen and big holes mesh for one layer then finish and heating by 120℃ -150℃ for 6-12 seconds , Heating time depends on drying temp