Preparation:

1.Mesh&Squeegee: 100-120(40-48T) Mesh number ;65-75 degree Squeegee.

2.Pigments added ratio:For white and fluorescent color 20%,other color 10% Chameleon ,Thermochromic Glitter powders ,mixing ratio 3-10%.

3.Catalyst mixing ratio:2% slow dry XG-866B-1 and fast dry XG-866B-2 can mix together for using.

4.Thinner XG-128A adding ratio:0-20% .

5.Heating Temp and time: Flash cure temp :100℃- 120℃ for 6-10 seconds,Drying temp :120℃- 130℃ for about 2 -3 minutes.

Silicone paste printing tips:

1.HD silicone XG-866A/866AH for under coating and high density printing for 2

times

HD silicone XG-866A/866AH 50G

Fast dry catalyst XG-866B-2 1G 2% If machine printing to use slow dry catalyst.

Silicone thinner XG-128AH thinner is not necessary for hand printing,5-20% is enough for machine printing.

Cure by temp of 120℃ 6-10 seconds. If fabric with hairy or want to get more smoth effect kindly assist by heat press machine or iron after first time printing. After printing keep wet to heat press by temp 150-170 degree for 10-20 seconds.