Anti slip socks silicone paste New socks silicone paste testing
Preparation
1.Mesh: 30-60(12T-24T) to make thick screen by emulsion.Better to use Hollow aluminum plate as showed on video.
2.Pigments added ratio:2-4%
3.Catalyst mixing ratio:2%
4.Thinner XG-128AH adding ratio:thinner is not necessary
5.Heating Temp and time: 120℃ -150℃ for 6-12 seconds , Heating time depends on drying temp.
Silicone paste mixing tips
Socks silicone XG-15A+ 60G
Catalyst XG-15B+1.2G (2%)
Pigment XG- 1.2-2.4G (2-4%) If need color effect
To print by thick screen and big holes mesh for one layer then finish and heating by 120℃ -150℃ for 6-12 seconds , Heating time depends on drying temp