1.To mix wiht silicone and catalyst ,printing 2 times for under

coating,first time to heat press by heat press machine to cure and get smooth effect ,the second time to flash by temp 120 degree.Heat press temp 150-190 degree,8-20 seconds depends on printing size and machine

HD silicone XG-866A 60G

Fast dry catalyst XG-866B-2 1.2G

2.Flash temp 110-120 degree ,To print anti-migration silicone for 2-3 times

Anti-migration silicone XG-866F 50G

Fast dry catalyst 1G 2%

3.To mix wiht HD silicone and catalyst print 2-4 times for high denslty ,Flash temp 120 degree

HD silicone XG-866A 50G

Fast dry catalyst XG-866B-2 1G 2%

4.To mix wiht HD silicone and catalyst , pigment,Printing 3-4 times ,if other colors 10%,Flash temp 120 degree

HD silicone XG-866A 60G

Fast dry catalyst 1.2G 2%

White pigment XG-102 12G 20%