Preparation:
1.Mesh&Squeegee: 120(48T) Mesh number ;65-75 degree Squeegee.
2. Pigments added ratio:For white and fluorescent color 20%,other color 10%
3.Catalyst mixing ratio:10% slow dry XG-MB-1 Extra slow dry catalyst XG-TMB-1
4.Silicone thinner XG-128AH adding ratio:0-20%
5.Heating Temp :60℃~100℃
Printing process:
1.PU based for under printing for 4-6 layers to get smooth layer first
HD PU water based nylon Ink XGS-806 100 G
Fixer XGS-339 2G 2% Flash by 80℃- 100℃.
Have to make sure to get PU based 100% dry and clear first,then move to print silicone crossing linker and silicone ink or will lead crossing linker and silicone ink not easy to dry and layers peal off from PU based ink .
2.Silicone crossing linker for mid layer printing for 2 layers
Silicone crossing linker XG-360Z-3X 50G
Silicone catalyst XG-866B-2+ 3-4G 6-8% Flash by 100-120 ℃