Preparation:
Mesh&Squeegee:120(48T)
Mesh number ;65-75 degree Squeegee.
Pigments added ratio:For white and fluorescent color 20%,other color 10%
Catalyst mixing ratio:2%slow dry XG-866B-I and fast dry XG-866B-2 can mix toge ther for using.Thinner XG-128A adding ratio:0-20% thinner is not necessary for hand printing HeatingTemp and time:Flash cure temp:100°℃-120°℃ for 6-10 seconds,Drying temp:120°℃-140℃ for about 2-5 minutes.
Silicone ink printing tips:
1 ,HD silicone XG-866A/866AH for under coating and high density printing for 2-8 times:
HD silicone XG-866A/866AH 60G
Fast dry catalyst XG-866B-21.2G 2%If machine printing to use slow dry catalyst.
Thinner XG-128AH thinner is not necessary for hand printing5-20%is enough for machine printing.Cure by temp of 120°C 6-10seconds
If fabrie with hairy or want to get mare smooth erfect kindly assist by heat press machine or iron after first time printing After printingkeep wet to heat press by temp 150-170 degree for 10-20 seconds.
2.Color e fleet silicone printing for 3-4 times :
HD silicone XG-866A/866AH 50G
White color pigment XG-10210G For white and fluorescent color 20%,other color 10%Fast dry catalyst XG-866B-2 IG 2%If machine printing to use slow dry catalyst.
Thinner XG-128AH thinner is not necessary for hand printing5-10%is enough for machine printing.Cure by temp of 120°C 6-10seconds
3.Glossy silicone ink or matte silicone ink for top coating:
Glossy top coating for 1-2 times:
Glossy silicone ink XG-399-350G
Fast dry catalyst XG-866B-21G 2%It will be better to use slow dry catalyst XG-866B-1 for machine printing.
Thinner XG-128AH thinner is not necessary for hand printing,5-10%is enough for machine printing.Cure by temp of 100-110℃10-25 seconds Have to get silicone bubbles out first,try to use code wind to support and it will be better to use low temp by longerheating time to avoid bubbles problem.